| Product Name | Heat-resisting Steel Electrode | |||||||
| Product No. | MMDE411-WE044 | |||||||
| Standard | ||||||||
| GB | AWS | JIS | DIN | |||||
| E5515-B2-V | E8016-B2 | DT2315 | ||||||
| Type of Covering | Low hydrogen Sodium | |||||||
| Welding Position | F,V, OH,H | |||||||
| Chemical Composition of Deposited Metal (%) | ||||||||
| Chemical Composition | C | Mn | Si | S | P | Cr | Mo | V |
| Standard | 0.05-0.12 | ≤0.90 | ≤0.60 | ≤0.035 | ≤0.035 | 0.80-1.50 | 0.40-0.65 | 0.10-0.35 |
| Typical | 0.066 | 0.70 | 0.37 | 0.012 | 0.015 | 1.12 | 0.52 | 0.18 |
| Mechanical Properties of Deposited Metal | ||||||||
| Test Item | Tensile Strengh Rm (MPa) | Yield point ReL (MPa) | Elongation A4 (%) | Akv1(J) | ||||
| Standard | ≥540 | ≥440 | ≥17 | 25℃ ≥27 | ||||
| Typical | 640 | 540 | 23 | 150 | ||||
| Reference Current ( DC) | ||||||||
| Electrode Diameter(mm) | 2.0 | 2.5 | 3.2 | 5.0 | ||||
| Welding Current(A) | 40-70 | 60-90 | 90-120 | 170-210 | ||||
Instructions
| ||||||||
1.The Electrodes must be baked under 300~350 for an hour before Welding and used as soon as baking is completed.
| ||||||||
2.The stains on the weldments, such as rust, oil stains, moisture, etc., must be cleared away before Welding.
| ||||||||
3.When Welding, short arc must be used and stringer bead is suitable.
| ||||||||
Application
| ||||||||
For welding low alloy CrMo pearlitic steels, such as high temperature, high presure boiler pipeline, petroleum cracking equipment, working temperature of which is below 540 ℃. | ||||||||